Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® B3S R03 - PA6 - BASF

Material Data Center offers the following functions for Ultramid® B3S R03:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Ultramid B datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
用于快速加工的易流动、 精细结晶注塑等级。 用途包括薄壁技术零部件 (例如外壳、 配件、 把手、 小型零部件、 锚和固定夹具)。
加工/物理特性干 / 已调节单位Test Standard
ISO数据
熔体体积流动速度, MVR 190 / * cm³/10min ISO 1133
温度 275 / * °C -
载荷 5 / * kg -
模塑收缩率, 平行 0.9 / * % ISO 294-4, 2577
模塑收缩率, 垂直 1.0 / * % ISO 294-4, 2577
喷射温度 145 °C -
机械性能干 / 已调节单位Test Standard
ISO数据
拉伸模量 3500 / 1200 MPa ISO 527
屈服应力 90 / 45 MPa ISO 527
屈服伸长率 4 / 20 % ISO 527
名义断裂伸长率 10 / >50 % ISO 527
弯曲模量, 23°C 3000 / - MPa ISO 178
拉伸蠕变模量, 1h * / 1300 MPa ISO 899-1
拉伸蠕变模量, 1000h * / 1100 MPa ISO 899-1
无缺口简支梁冲击强度, +23°C 250 / N kJ/m² ISO 179/1eU
简支梁冲击强度, -30°C 200 / - kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C 4 / 50 kJ/m² ISO 179/1eA
简支梁缺口冲击强度, -30°C 3 / - kJ/m² ISO 179/1eA
热性能干 / 已调节单位Test Standard
ISO数据
熔融温度, 10°C/min 220 / * °C ISO 11357-1/-3
玻璃化转变温度, 10°C/min 60 / * °C ISO 11357-1/-2
热变形温度, 1.80 MPa 65 / * °C ISO 75-1/-2
热变形温度, 0.45 MPa 180 / * °C ISO 75-1/-2
线性热膨胀系数, 平行 102 / * E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 V-2 / * class IEC 60695-11-10
测试用试样的厚度 1.6 / * mm -
Yellow Card 现存 是的 / * - -
厚度为h时的燃烧性 V-2 / * class IEC 60695-11-10
测试用试样的厚度 0.8 / * mm -
Yellow Card 现存 是的 / * - -
电性能干 / 已调节单位Test Standard
ISO数据
相对介电常数., 100Hz 4.1 / - - IEC 62631-2-1
相对介电常数., 1MHz 3.3 / 7 - IEC 62631-2-1
介质损耗因子, 100Hz 100 / - E-4 IEC 62631-2-1
介质损耗因子, 1MHz 300 / 3000 E-4 IEC 62631-2-1
体积电阻率 1E13 / 1E9 Ohm*m IEC 62631-3-1
表面电阻率 * / 1E12 Ohm IEC 62631-3-2
介电强度 40 / 29 kV/mm IEC 60243-1
相对漏电起痕指数 - / 600 - IEC 60112
其它性能干 / 已调节单位Test Standard
吸水性 9.5 / * % 类似ISO 62
吸湿性 3 / * % 类似ISO 62
密度 1130 / - kg/m³ ISO 1183
Bulk density 700 kg/m³ -
模塑测量的特殊性能干 / 已调节单位Test Standard
ISO数据
粘数 145 / * cm³/g ISO 307, 1157, 1628
试样制备条件价值单位Test Standard
ISO数据
注塑, 熔体温度 260 °C ISO 294
注塑, 模具温度 80 °C ISO 294
注塑, 注射速度 200 mm/s ISO 294
加工推荐(注塑)价值单位Test Standard
预干燥-温度 80 °C -
预干燥-时间 4 h -
加工湿度 ≤0.15 % -
注塑熔体温度 250 - 270 °C -
模具温度 40 - 60 °C -
典型数据
加工方法
注塑
供货形式
粒料
添加剂
润滑剂, 脱模助剂
特征
少气味
应用
封装
地区供应
欧洲
其他信息
注塑成型
PREPROCESSING
Pre/Post-processing, max. allowed water content: .15 %
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 250 - 270 °C
injection molding, Melt temperature, recommended: 260 °C
injection molding, Mold temperature, range: 40 - 60 °C
injection molding, Mold temperature, recommended: 60 °C
injection molding, Dwell time, thermoplastics: 10 min
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.